Pages 55-59, Language: EnglishImbery / DavisThe tensile bond strength of Panavia EX to a high-noble alloy prepared by abrasive spraying and tin plating was measured Two different intraoperatory tin plating systems were compared. Disk-shaped specimens were cast in type III gold, abrasive sprayed with aluminum oxide, and divided into three groups of 30 specimens each. Specimens in one group were tin plated by using a Kura Ace Mini unit, those in the second group were tin plated by using a Micro Tin unit, and those in the third group were not tin plated and served as the control group. Disks within each group were luted to each other with Panavia EX. The specimens were thermocycled and tested in tension. There was no significant difference between the two tin plated groups; however, the luting bond of both experimental groups was significantly stronger than was that of the control (P .05).