DOI: 10.11607/ijp.3686, PubMed-ID: 24905269Seiten: 267-269, Sprache: EnglischCanullo, Luigi / Micarelli, Costanza / Bettazzoni, Laura / Koçi, Brunilda / Baldissara, PaoloPurpose: To compare the shear bond strength (SBS) values of resin cement to zirconia treated with a new activating method.
Materials and Methods: Forty-five zirconia specimens were divided into three groups: no treatment (group 1), plasma of argon cleaning for 375 seconds (group 2), and plasma of argon cleaning for 750 seconds (group 3). Composite cylinders were bonded with a self-adhesive cement. After 40 days of water storage, specimens were subjected to the SBS test. Data were analyzed with one-way analysis of variance and the Neuman-Keuls multiple comparison test.
Results: Test groups obtained SBS values significantly higher (101% for group 2 and 81% for group 3) than controls.